What 1.4408 is
1.4408 is the material number of GX5CrNiMo19-11-2, an austenitic cast stainless steel in EN 10213. In the name, G marks a casting, X a high-alloy steel, 5 the nominal carbon content in hundredths of a percent, and CrNiMo19-11-2 the nominal chromium, nickel and molybdenum contents in percent. It is the usual European counterpart of ASTM CF8M (cast 316).
1.4408 equivalents: ASTM, China and Russia
Scroll sideways to see the whole table
| Standard | Grade | Note |
|---|---|---|
| ASTM A351 (USA) | CF8M | Carbon up to 0.08%, molybdenum 2.0–3.0% |
| Wrought counterpart | 316 | Composition limits and structure differ from the cast grade |
| GB/T 2100-2017 (China) | ZG07Cr19Ni11Mo2 | Nearest Chinese corrosion-resistant casting grade |
| ГОСТ 977-88 (Russia) | 12Х18Н12М3ТЛ | Nearest by composition; titanium-stabilised, carbon up to 0.12%, molybdenum 3.0–4.0% |
These equivalents are approximate, not identical materials. Composition limits, test methods and heat treatment differ between standards. The standard named on the drawing governs, and any substitution needs the buyer’s written approval.
1.4408 chemical composition
Scroll sideways to see the whole table
| Element | 1.4408 (EN 10213) | CF8M (ASTM A351) |
|---|---|---|
| Carbon (C) | 0.07 | 0.08 |
| Silicon (Si) | 1.50 | 1.50 |
| Manganese (Mn) | 1.50 | 1.50 |
| Phosphorus (P) | 0.040 | 0.040 |
| Sulfur (S) | 0.030 | 0.040 |
| Chromium (Cr) | 18.0–20.0 | 18.0–21.0 |
| Nickel (Ni) | 9.0–12.0 | 9.0–12.0 |
| Molybdenum (Mo) | 2.0–2.5 | 2.0–3.0 |
| Copper (Cu) | 0.50 | – |
1.4408 mechanical properties
Scroll sideways to see the whole table
| Grade | Tensile, MPa | Yield, MPa | Elongation, % |
|---|---|---|---|
| 1.4408 (EN 10213) | 440–640 | 210 (Rp1.0) | 30 |
| CF8M (ASTM A351) | 485 | 205 (0.2%) | 30 |
EN 10213 values are for the solution-annealed condition (+AT) and wall thicknesses up to 150 mm. EN 10213 states a 1% proof strength (Rp1.0) for austenitic grades, which is not the same measure as the ASTM 0.2% yield strength.
EN 10213 also requires a minimum impact energy (KV) of 60 J at room temperature for 1.4408.
Heat treatment and welding
Heat treatment. EN 10213 lists 1.4408 as solution annealed (+AT) at 1080–1150 °C, followed by quenching in water.
Where parts are welded and corrosion resistance next to the weld matters, the low-carbon grade 1.4409 (GX2CrNiMo19-11-2, the counterpart of CF3M) is often specified instead.
How JK Casting makes 1.4408 castings
JK Casting reviews every stainless steel casting part by part. Send the drawing, the grade with its standard and any corrosion or test requirements, and JK confirms the casting route, investment casting or sand casting, before quoting. Investment castings made in-house weigh up to about 20 kg each. Castings are supplied raw or machined, and JK machines only the castings it makes. Each drawing is quoted separately, with tooling and unit price on separate lines.
Related pages: Cast stainless steel grades chart · Investment casting · Steel castings · What to put on a casting drawing · Send a drawing for quotation
Frequently asked questions
Is 1.4408 the same as CF8M?
They are the usual counterparts but not identical. 1.4408 allows up to 0.07% carbon and 2.0–2.5% molybdenum; CF8M allows up to 0.08% carbon and 2.0–3.0% molybdenum. The drawing’s standard governs.
What is the difference between 1.4408 and 1.4409?
1.4409 (GX2CrNiMo19-11-2) is the low-carbon version: carbon up to 0.030% against 0.07%, with nitrogen up to 0.20%. It is the counterpart of CF3M.
What does GX5CrNiMo19-11-2 mean?
G marks a casting, X a high-alloy steel, 5 the nominal carbon content in hundredths of a percent, and 19-11-2 the nominal chromium, nickel and molybdenum contents in percent.
Standards referenced: EN 10213; ASTM A351/A351M; GB/T 2100-2017; ГОСТ 977-88.