CF8 Stainless Steel (Cast 304): Equivalents, Composition and Properties

CF8 is an austenitic cast stainless steel grade in ASTM A351 and A743, the cast counterpart of wrought 304: carbon up to 0.08%, chromium 18.0–21.0%, nickel 8.0–11.0%. This page compares it with 1.4308, ZG07Cr19Ni10 and the ГОСТ grades and lists its composition and properties.

JK Casting · Buyer resource · Updated 16 November 2026

What CF8 is

CF8 is the cast counterpart of 304 stainless steel. It is defined in ASTM A351 (castings for pressure-containing parts) and also listed in ASTM A743 (general-service corrosion-resistant castings). It is an austenitic chromium-nickel steel without molybdenum; where pitting resistance is needed, CF8M is the molybdenum-bearing alternative.

CF8 equivalents: China, Europe and Russia

Scroll sideways to see the whole table

Approximate comparison. The standard on the drawing governs; substitution needs buyer approval.
StandardGradeNote
Wrought counterpart304Composition limits and structure differ from the cast grade
GB/T 2100-2017 (China)ZG07Cr19Ni10Nearest Chinese corrosion-resistant casting grade
EN 10213 (Europe)1.4308 (GX5CrNi19-10)Carbon ≤0.07%, chromium 18.0–20.0%
ГОСТ 977-88 (Russia)10Х18Н9ЛNearest by composition; carbon up to 0.14%
ГОСТ 977-88 (Russia)12Х18Н9ТЛTitanium-stabilised; carbon up to 0.12%

These equivalents are approximate, not identical materials. Composition limits, test methods and heat treatment differ between standards. The standard named on the drawing governs, and any substitution needs the buyer’s written approval.

CF8 chemical composition

Scroll sideways to see the whole table

% by mass; single values are maximums.
ElementCF8 (ASTM A351)1.4308 (EN 10213)
Carbon (C)0.080.07
Silicon (Si)2.001.50
Manganese (Mn)1.501.50
Phosphorus (P)0.0400.040
Sulfur (S)0.0400.030
Chromium (Cr)18.0–21.018.0–20.0
Nickel (Ni)8.0–11.08.0–11.0
Molybdenum (Mo)0.50–
Copper (Cu)–0.50

CF8 mechanical properties

Scroll sideways to see the whole table

Minimum values unless a range is shown.
GradeTensile, MPaYield, MPaElongation, %
CF8 (ASTM A351)485205 (0.2%)35
1.4308 (EN 10213)440–640200 (Rp1.0)30
10Х18Н9Л (ГОСТ 977-88)44117725

ASTM A351 covers austenitic castings for pressure-containing parts; ASTM A743 lists the same grade names for general-service corrosion-resistant castings. Tensile values are minimums from ASTM A351; elongation is measured over 50 mm. In ksi: tensile 70, yield 30.

EN 10213 values are for the solution-annealed condition (+AT) and wall thicknesses up to 150 mm. EN 10213 states a 1% proof strength (Rp1.0) for austenitic grades, which is not the same measure as the ASTM 0.2% yield strength.

Heat treatment and welding

Heat treatment. ASTM A351 requires these grades to be solution annealed at 1040 °C (1900 °F) minimum, then quenched in water or rapidly cooled by other means. Weld repairs are made with procedures and welders qualified to ASTM A488.

ГОСТ 977-88 gives quenching from 1060–1100 °C in water, oil or air for 10Х18Н9Л. CF8 welds readily; where corrosion resistance next to welds is critical, the low-carbon grade CF3 (cast 304L) is often specified instead.

How JK Casting makes CF8 castings

JK Casting reviews every stainless steel casting part by part. Send the drawing, the grade with its standard and any corrosion or test requirements, and JK confirms the casting route, investment casting or sand casting, before quoting. Investment castings made in-house weigh up to about 20 kg each. Castings are supplied raw or machined, and JK machines only the castings it makes. Each drawing is quoted separately, with tooling and unit price on separate lines.

Related pages: Cast stainless steel grades chart · Investment casting · Steel castings · What to put on a casting drawing · Send a drawing for quotation

Frequently asked questions

Is CF8 the same as 304?

No. CF8 is the cast counterpart of wrought 304. Its composition limits differ, for example chromium 18.0–21.0% in ASTM A351, and the cast structure normally contains some ferrite.

What is the difference between CF8 and CF3?

CF3 allows at most 0.03% carbon against 0.08% for CF8. It is the cast counterpart of 304L and is chosen when parts are welded and corrosion resistance next to the weld matters.

What is the European equivalent of CF8?

EN 10213 1.4308 (GX5CrNi19-10) is the usual counterpart. It allows up to 0.07% carbon and 18.0–20.0% chromium. The equivalence is approximate.

What is the Chinese equivalent of CF8?

The nearest GB/T 2100-2017 grade is ZG07Cr19Ni10. The equivalence is approximate, so the drawing’s standard governs and a substitution needs approval.

Standards referenced: ASTM A351/A351M; ASTM A743/A743M; EN 10213; GB/T 2100-2017; ГОСТ 977-88.