CF3 Stainless Steel (Cast 304L): Equivalents, Composition and Properties

CF3 is the low-carbon austenitic cast stainless steel grade in ASTM A351 and A743, the cast counterpart of wrought 304L: carbon up to 0.03%, chromium 17.0–21.0%, nickel 8.0–12.0%. This page compares it with 1.4309 and ZG03Cr19Ni11 and lists its composition and properties.

JK Casting · Buyer resource · Updated 16 November 2026

What CF3 is

CF3 is the cast counterpart of 304L stainless steel. It is defined in ASTM A351 and also listed in ASTM A743. The 3 means at most 0.03% carbon. Low carbon reduces carbide precipitation next to welds, so CF3 is chosen instead of CF8 for welded parts where corrosion resistance at the weld matters.

CF3 equivalents: China, Europe and Russia

Scroll sideways to see the whole table

Approximate comparison. The standard on the drawing governs; substitution needs buyer approval.
StandardGradeNote
Wrought counterpart304LComposition limits and structure differ from the cast grade
GB/T 2100-2017 (China)ZG03Cr19Ni11Nearest Chinese corrosion-resistant casting grade
EN 10213 (Europe)1.4309 (GX2CrNi19-11)Carbon ≤0.030%, chromium 18.0–20.0%, nitrogen ≤0.20%
ГОСТ 977-88 (Russia)No direct equivalentNo austenitic grade with carbon at or below 0.03%

These equivalents are approximate, not identical materials. Composition limits, test methods and heat treatment differ between standards. The standard named on the drawing governs, and any substitution needs the buyer’s written approval.

CF3 chemical composition

Scroll sideways to see the whole table

% by mass; single values are maximums.
ElementCF3 (ASTM A351)1.4309 (EN 10213)
Carbon (C)0.030.030
Silicon (Si)2.001.50
Manganese (Mn)1.502.00
Phosphorus (P)0.0400.035
Sulfur (S)0.0400.025
Chromium (Cr)17.0–21.018.0–20.0
Nickel (Ni)8.0–12.09.0–12.0
Molybdenum (Mo)0.50–
Nitrogen (N)–0.20

CF3 mechanical properties

Scroll sideways to see the whole table

Minimum values unless a range is shown.
GradeTensile, MPaYield, MPaElongation, %
CF3 (ASTM A351)485205 (0.2%)35
1.4309 (EN 10213)440–640210 (Rp1.0)30

ASTM A351 covers austenitic castings for pressure-containing parts; ASTM A743 lists the same grade names for general-service corrosion-resistant castings. Tensile values are minimums from ASTM A351; elongation is measured over 50 mm. In ksi: tensile 70, yield 30.

EN 10213 values are for the solution-annealed condition (+AT) and wall thicknesses up to 150 mm. EN 10213 states a 1% proof strength (Rp1.0) for austenitic grades, which is not the same measure as the ASTM 0.2% yield strength.

Heat treatment and welding

Heat treatment. ASTM A351 requires these grades to be solution annealed at 1040 °C (1900 °F) minimum, then quenched in water or rapidly cooled by other means. Weld repairs are made with procedures and welders qualified to ASTM A488.

Because of its low carbon content, CF3 is the usual choice when castings are welded into an assembly and the weld area must keep its corrosion resistance.

How JK Casting makes CF3 castings

JK Casting reviews every stainless steel casting part by part. Send the drawing, the grade with its standard and any corrosion or test requirements, and JK confirms the casting route, investment casting or sand casting, before quoting. Investment castings made in-house weigh up to about 20 kg each. Castings are supplied raw or machined, and JK machines only the castings it makes. Each drawing is quoted separately, with tooling and unit price on separate lines.

Related pages: Cast stainless steel grades chart · Investment casting · Steel castings · What to put on a casting drawing · Send a drawing for quotation

Frequently asked questions

Is CF3 the same as 304L?

No. CF3 is the cast counterpart of wrought 304L. Its composition limits differ, for example chromium 17.0–21.0% in ASTM A351, and the cast structure normally contains some ferrite.

What is the difference between CF3 and CF8?

CF3 allows at most 0.03% carbon against 0.08% for CF8. Both have the same ASTM A351 tensile minimums (485 MPa tensile, 205 MPa yield, 35% elongation).

What is the European equivalent of CF3?

EN 10213 1.4309 (GX2CrNi19-11) is the usual counterpart. It allows up to 0.030% carbon and 18.0–20.0% chromium. The equivalence is approximate.

Is there a Russian equivalent of CF3?

ГОСТ 977-88 lists no austenitic casting grade with carbon at or below 0.03%, so there is no direct equivalent. Agree the grade and standard on the drawing.

Standards referenced: ASTM A351/A351M; ASTM A743/A743M; EN 10213; GB/T 2100-2017; ГОСТ 977-88.