What CF8M is
CF8M is the cast counterpart of 316 stainless steel. It is defined in ASTM A351 (castings for pressure-containing parts) and also listed in ASTM A743 (general-service corrosion-resistant castings). The M stands for molybdenum, 2.0–3.0%, which improves resistance to pitting compared with CF8.
CF8M equivalents: China, Europe and Russia
Scroll sideways to see the whole table
| Standard | Grade | Note |
|---|---|---|
| Wrought counterpart | 316 | Composition limits and structure differ from the cast grade |
| GB/T 2100-2017 (China) | ZG07Cr19Ni11Mo2 | Nearest Chinese corrosion-resistant casting grade |
| EN 10213 (Europe) | 1.4408 (GX5CrNiMo19-11-2) | Carbon ≤0.07%, molybdenum 2.0–2.5% |
| ГОСТ 977-88 (Russia) | 12Х18Н12М3ТЛ | Nearest by composition; titanium-stabilised, carbon up to 0.12%, molybdenum 3.0–4.0% |
These equivalents are approximate, not identical materials. Composition limits, test methods and heat treatment differ between standards. The standard named on the drawing governs, and any substitution needs the buyer’s written approval.
CF8M chemical composition
Scroll sideways to see the whole table
| Element | CF8M (ASTM A351) | 1.4408 (EN 10213) |
|---|---|---|
| Carbon (C) | 0.08 | 0.07 |
| Silicon (Si) | 1.50 | 1.50 |
| Manganese (Mn) | 1.50 | 1.50 |
| Phosphorus (P) | 0.040 | 0.040 |
| Sulfur (S) | 0.040 | 0.030 |
| Chromium (Cr) | 18.0–21.0 | 18.0–20.0 |
| Nickel (Ni) | 9.0–12.0 | 9.0–12.0 |
| Molybdenum (Mo) | 2.0–3.0 | 2.0–2.5 |
| Copper (Cu) | – | 0.50 |
CF8M mechanical properties
Scroll sideways to see the whole table
| Grade | Tensile, MPa | Yield, MPa | Elongation, % |
|---|---|---|---|
| CF8M (ASTM A351) | 485 | 205 (0.2%) | 30 |
| 1.4408 (EN 10213) | 440–640 | 210 (Rp1.0) | 30 |
| 12Х18Н12М3ТЛ (ГОСТ 977-88) | 441 | 216 | 25 |
ASTM A351 covers austenitic castings for pressure-containing parts; ASTM A743 lists the same grade names for general-service corrosion-resistant castings. Tensile values are minimums from ASTM A351; elongation is measured over 50 mm. In ksi: tensile 70, yield 30.
EN 10213 values are for the solution-annealed condition (+AT) and wall thicknesses up to 150 mm. EN 10213 states a 1% proof strength (Rp1.0) for austenitic grades, which is not the same measure as the ASTM 0.2% yield strength.
Heat treatment and welding
Heat treatment. ASTM A351 requires these grades to be solution annealed at 1040 °C (1900 °F) minimum, then quenched in water or rapidly cooled by other means. Weld repairs are made with procedures and welders qualified to ASTM A488.
ГОСТ 977-88 gives quenching from 1100–1150 °C in water for 12Х18Н12М3ТЛ. Where parts are welded and corrosion resistance next to the weld matters, the low-carbon grade CF3M (cast 316L) is often specified instead.
How JK Casting makes CF8M castings
JK Casting reviews every stainless steel casting part by part. Send the drawing, the grade with its standard and any corrosion or test requirements, and JK confirms the casting route, investment casting or sand casting, before quoting. Investment castings made in-house weigh up to about 20 kg each. Castings are supplied raw or machined, and JK machines only the castings it makes. Each drawing is quoted separately, with tooling and unit price on separate lines.
Related pages: Cast stainless steel grades chart · Investment casting · Steel castings · What to put on a casting drawing · Send a drawing for quotation
Frequently asked questions
Is CF8M the same as 316?
No. CF8M is the cast counterpart of wrought 316. Its composition limits differ, for example chromium 18.0–21.0% in ASTM A351, and the cast structure normally contains some ferrite. If a drawing for a cast part names 316, agree the casting grade in writing.
What is the difference between CF8M and CF3M?
CF3M allows at most 0.03% carbon against 0.08% for CF8M, and a slightly wider nickel range. It is the cast counterpart of 316L and is chosen for welded parts where corrosion resistance next to the weld matters.
What is the European equivalent of CF8M?
EN 10213 1.4408 (GX5CrNiMo19-11-2) is the usual counterpart. It allows up to 0.07% carbon and 2.0–2.5% molybdenum, a narrower range than CF8M’s 2.0–3.0%.
What is the Russian equivalent of CF8M?
ГОСТ 977-88 12Х18Н12М3ТЛ is the nearest by composition, but it is titanium-stabilised, allows up to 0.12% carbon and has 3.0–4.0% molybdenum, so it is not a direct equivalent.
Standards referenced: ASTM A351/A351M; ASTM A743/A743M; EN 10213; GB/T 2100-2017; ГОСТ 977-88.