12Х18Н9ТЛ (12Kh18N9TL) Cast Stainless Steel to ГОСТ 977: Composition, Properties and Equivalents

12Х18Н9ТЛ is a titanium-stabilised austenitic corrosion-resistant casting steel in the Russian standard ГОСТ 977-88: carbon up to 0.12%, chromium 17–20%, nickel 8–11%. This page explains the name and gives its composition, properties and heat treatment and the grades it is compared with.

JK Casting · Buyer resource · Updated 16 November 2026

What 12Х18Н9ТЛ is

12Х18Н9ТЛ is an austenitic corrosion-resistant casting steel in ГОСТ 977-88. In the name, 12 refers to the carbon content in hundredths of a percent (here at most 0.12%), Х18 to about 18% chromium, Н9 to about 9% nickel, Т to titanium and Л to a casting steel (литейная). ГОСТ 977-88 describes it as corrosion-resistant, heat-resistant up to 750 °C and creep-resistant up to 600 °C, with high resistance to gas and intergranular corrosion.

12Х18Н9ТЛ equivalents and nearest grades

Scroll sideways to see the whole table

Approximate comparison. The standard on the drawing governs; substitution needs buyer approval.
StandardGradeNote
ГОСТ 977-88 (Russia)10Х18Н9ЛSame family without titanium; carbon up to 0.14%
ASTM A351 (USA)CF8Carbon up to 0.08%, no titanium
EN 10213 (Europe)1.4308 (GX5CrNi19-10)Carbon up to 0.07%, no titanium

These equivalents are approximate, not identical materials. Composition limits, test methods and heat treatment differ between standards. The standard named on the drawing governs, and any substitution needs the buyer’s written approval.

The titanium addition stabilises 12Х18Н9ТЛ against intergranular corrosion; the ASTM and EN grades in this table are not titanium-stabilised, so they are comparisons, not equivalents.

12Х18Н9ТЛ chemical composition

Scroll sideways to see the whole table

ГОСТ 977-88, Table 2.
ElementContent, % by mass
Carbon (C)≤0.12
Silicon (Si)0.20–1.00
Manganese (Mn)1.00–2.00
Chromium (Cr)17.0–20.0
Nickel (Ni)8.00–11.00
Titanium (Ti)5 × C to 0.70
Sulfur (S)≤0.030
Phosphorus (P)≤0.035

12Х18Н9ТЛ mechanical properties

Scroll sideways to see the whole table

ГОСТ 977-88: minimum values.
GradeYield, MPaTensile, MPaElongation, %Reduction of area, %
12Х18Н9ТЛ (ГОСТ 977-88)1964412532
10Х18Н9Л (ГОСТ 977-88)1774412535

Impact values are left out of this table; if the part needs an impact test, state the test and temperature on the drawing.

Heat treatment and welding

Heat treatment. ГОСТ 977-88 gives quenching from 1050–1100 °C with cooling in water, oil or air for 12Х18Н9ТЛ.

Titanium ties up carbon, which helps the steel keep its resistance to intergranular corrosion after heating, for example near welds.

How JK Casting makes 12Х18Н9ТЛ castings

JK Casting reviews every stainless steel casting part by part. Send the drawing, the grade with its standard and any corrosion or test requirements, and JK confirms the casting route, investment casting or sand casting, before quoting. Investment castings made in-house weigh up to about 20 kg each. Castings are supplied raw or machined, and JK machines only the castings it makes. Each drawing is quoted separately, with tooling and unit price on separate lines.

Related pages: Cast stainless steel grades chart · Investment casting · Steel castings · What to put on a casting drawing · Send a drawing for quotation

Frequently asked questions

What does 12Х18Н9ТЛ mean?

12 refers to the carbon content in hundredths of a percent (at most 0.12%), Х18 to about 18% chromium, Н9 to about 9% nickel, Т to titanium, and Л to a casting steel. The grade is defined in ГОСТ 977-88.

What is the ASTM equivalent of 12Х18Н9ТЛ?

There is no direct equivalent. CF8 is the nearest common cast grade by chromium and nickel content, but it is not titanium-stabilised and allows less carbon (0.08%). The comparison is approximate.

What is the chemical composition of 12Х18Н9ТЛ?

Carbon up to 0.12%, silicon 0.20–1.00%, manganese 1.00–2.00%, chromium 17.0–20.0%, nickel 8.00–11.00%, titanium from 5 times the carbon content up to 0.70%, sulfur up to 0.030% and phosphorus up to 0.035%.

How is 12Х18Н9ТЛ heat treated?

ГОСТ 977-88 gives quenching from 1050–1100 °C with cooling in water, oil or air. The minimums are then 196 MPa yield, 441 MPa tensile and 25% elongation.

Standards referenced: ГОСТ 977-88; ASTM A351/A351M; EN 10213.