Custom castings from your drawings or samples. Send your requirements for a quotation.Request a Quote
Jiangkai Casting logoJK CastingDrawing-based OEM metal parts

Material reference

20L (20Л) Cast Steel to ГОСТ 977: Equivalents, Composition and Properties

20Л (often written 20L) is a low-carbon cast steel grade in the Russian standard ГОСТ 977-88. 20 is the average carbon content in hundredths of a percent; Л marks a casting steel. This page gives its composition, properties and heat treatment and the grades it is compared with.

JK Casting · Buyer resource · Updated 16 November 2026

What 20Л is

20Л is an unalloyed structural casting steel in ГОСТ 977-88. 20 is the average carbon content in hundredths of a percent (carbon 0.17–0.25%); Л stands for литейная, casting steel. ГОСТ 977 sorts castings into groups 1–3 (general, responsible and especially responsible duty); the group sets the checks and the sulfur and phosphorus limits, so state it on the drawing.

20Л equivalents and nearest grades

Scroll sideways to see the whole table

Approximate comparison. The standard on the drawing governs; substitution needs buyer approval.
GradeStandardMin. yield, MPaTensile, MPaMin. elongation, %How it compares
20ЛГОСТ 977 (Russia), normalised216412 min.22Reference grade
ZG200-400GB/T 11352 (China)200400 min.25Lower minimum yield and tensile strength, higher minimum elongation
25ЛГОСТ 977 (Russia), normalised235441 min.19Higher carbon: higher strength, lower elongation

These equivalents are approximate, not identical materials. Composition limits, test methods and heat treatment differ between standards. The standard named on the drawing governs, and any substitution needs the buyer’s written approval.

20Л chemical composition

Scroll sideways to see the whole table

ГОСТ 977-88, Tables 1 and 4.
ElementContent, % by mass
Carbon (C)0.17–0.25
Manganese (Mn)0.45–0.90
Silicon (Si)0.20–0.52
Sulfur (S), groups 2 and 3≤0.045
Phosphorus (P), groups 2 and 3≤0.040
Sulfur (S), group 1≤0.050
Phosphorus (P), group 1≤0.050

Sulfur and phosphorus limits shown are for steel made by the basic process; ГОСТ 977 allows higher limits for acid and converter steel. Check the casting group and process stated for the order.

20Л mechanical properties

Scroll sideways to see the whole table

ГОСТ 977-88, Table 7: minimum values for castings with walls up to 100 mm.
ConditionMin. yield, MPaMin. tensile, MPaMin. elongation, %Min. reduction of area, %
Normalised, or normalised and tempered (К20)2164122235

ГОСТ 977-88 gives no quenched-and-tempered strength category for 20Л. Impact values are left out of this table; if the part needs an impact test, state the test and temperature on the drawing.

Heat treatment and welding

Heat treatment. ГОСТ 977-88 gives normalising at 880–900 °C for 20Л, or normalising at 880–900 °C followed by tempering at 630–650 °C.

Welding. With carbon limited to 0.25%, 20Л is a readily weldable carbon steel; preheat and post-weld heat treatment depend on section thickness and the welding procedure.

How JK Casting makes 20Л castings

JK Casting makes carbon steel castings to customer drawings in Gaomi, Shandong, China. Parts are sand cast, including shell moulding in resin-coated sand, or made by lost-wax investment casting; investment castings made in-house weigh up to about 20 kg each. Castings are supplied raw or machined, and JK machines only the castings it makes. Each drawing is quoted separately, with tooling and unit price on separate lines.

For a quotation, send the drawing with the full grade designation and standard, the heat treatment condition and any tests the part needs. Material records such as EN 10204 3.1 certificates are provided when agreed for the order.

Related pages: Steel castings · Investment casting · Sand casting · What to put on a casting drawing · Send a drawing for quotation

Frequently asked questions

What does 20Л mean?

20 is the average carbon content in hundredths of a percent (carbon 0.17–0.25%), and Л stands for литейная, a casting steel. The grade is defined in ГОСТ 977-88.

What are the equivalents of 20Л?

GB/T 11352 ZG200-400 is often compared with it: 200 MPa yield, 400 MPa tensile and 25% elongation, against 216 MPa, 412 MPa and 22% for normalised 20Л. The comparison is approximate.

What is the chemical composition of 20Л?

Carbon 0.17–0.25%, manganese 0.45–0.90%, silicon 0.20–0.52%; sulfur and phosphorus limits depend on the casting group and steelmaking process, for example 0.045% sulfur and 0.040% phosphorus for basic-process steel in groups 2 and 3.

How is 20Л heat treated?

ГОСТ 977-88 gives normalising at 880–900 °C, or normalising at 880–900 °C followed by tempering at 630–650 °C. The minimums are then 216 MPa yield and 412 MPa tensile.

Standards referenced: ГОСТ 977-88; GB/T 11352-2009.