Custom castings from your drawings or samples. Send your requirements for a quotation.Request a Quote
Jiangkai Casting logoJK CastingDrawing-based OEM metal parts

Material reference

25L (25Л) Cast Steel to ГОСТ 977: Equivalents, Composition and Properties

25Л (often written 25L) is a cast carbon steel grade in the Russian standard ГОСТ 977-88. 25 is the average carbon content in hundredths of a percent; Л marks a casting steel. This page gives its composition, properties and heat treatment and the WCB and ZG grades it is compared with.

JK Casting · Buyer resource · Updated 16 November 2026

What 25Л is

25Л is an unalloyed structural casting steel in ГОСТ 977-88. 25 is the average carbon content in hundredths of a percent (carbon 0.22–0.30%); Л stands for литейная, casting steel. ГОСТ 977 sorts castings into groups 1–3 (general, responsible and especially responsible duty); the group sets the checks and the sulfur and phosphorus limits, so state it on the drawing.

25Л equivalents: WCB and ZG230-450

Scroll sideways to see the whole table

Approximate comparison. The standard on the drawing governs; substitution needs buyer approval.
GradeStandardMin. yield, MPaTensile, MPaMin. elongation, %How it compares
25ЛГОСТ 977 (Russia), normalised235441 min.19Reference grade
ZG230-450GB/T 11352 (China)230450 min.22Similar values: lower minimum yield, higher minimum tensile strength
WCBASTM A216 (USA)250485–65522Higher minimum yield and tensile strength

These equivalents are approximate, not identical materials. Composition limits, test methods and heat treatment differ between standards. The standard named on the drawing governs, and any substitution needs the buyer’s written approval.

25Л chemical composition

Scroll sideways to see the whole table

ГОСТ 977-88, Tables 1 and 4.
ElementContent, % by mass
Carbon (C)0.22–0.30
Manganese (Mn)0.45–0.90
Silicon (Si)0.20–0.52
Sulfur (S), groups 2 and 3≤0.045
Phosphorus (P), groups 2 and 3≤0.040
Sulfur (S), group 1≤0.050
Phosphorus (P), group 1≤0.050

Sulfur and phosphorus limits shown are for steel made by the basic process; ГОСТ 977 allows higher limits for acid and converter steel. Check the casting group and process stated for the order.

25Л mechanical properties

Scroll sideways to see the whole table

ГОСТ 977-88, Table 7: minimum values for castings with walls up to 100 mm.
ConditionMin. yield, MPaMin. tensile, MPaMin. elongation, %Min. reduction of area, %
Normalised, or normalised and tempered (К20)2354411930
Quenched and tempered (КТ30)2944912233

Impact values are left out of this table; if the part needs an impact test, state the test and temperature on the drawing.

Heat treatment and welding

Heat treatment. ГОСТ 977-88 gives these modes for 25Л: normalising at 880–900 °C and tempering at 610–630 °C, or quenching from 870–890 °C and tempering at 610–630 °C.

Welding. With carbon limited to 0.30%, 25Л is a weldable carbon steel; preheat and post-weld heat treatment depend on section thickness and the welding procedure.

How JK Casting makes 25Л castings

JK Casting makes carbon steel castings to customer drawings in Gaomi, Shandong, China. Parts are sand cast, including shell moulding in resin-coated sand, or made by lost-wax investment casting; investment castings made in-house weigh up to about 20 kg each. Castings are supplied raw or machined, and JK machines only the castings it makes. Each drawing is quoted separately, with tooling and unit price on separate lines.

For a quotation, send the drawing with the full grade designation and standard, the heat treatment condition and any tests the part needs. Material records such as EN 10204 3.1 certificates are provided when agreed for the order.

Related pages: Steel castings · Investment casting · Sand casting · What to put on a casting drawing · Send a drawing for quotation

Frequently asked questions

What does 25Л mean?

25 is the average carbon content in hundredths of a percent (carbon 0.22–0.30%), and Л stands for литейная, a casting steel. The grade is defined in ГОСТ 977-88.

What are the equivalents of 25Л?

ASTM A216 WCB and GB/T 11352 ZG230-450 are the grades usually compared with it. ZG230-450 has similar values; WCB requires more (250 MPa yield, 485 MPa minimum tensile). The equivalence is approximate.

What is the chemical composition of 25Л?

Carbon 0.22–0.30%, manganese 0.45–0.90%, silicon 0.20–0.52%; sulfur and phosphorus limits depend on the casting group and steelmaking process, for example 0.045% sulfur and 0.040% phosphorus for basic-process steel in groups 2 and 3.

How is 25Л heat treated?

ГОСТ 977-88 gives normalising at 880–900 °C with tempering at 610–630 °C, or quenching from 870–890 °C with tempering at 610–630 °C. Normalised, the minimums are 235 MPa yield and 441 MPa tensile.

Standards referenced: ГОСТ 977-88; ASTM A216/A216M-21; GB/T 11352-2009.