Custom castings from your drawings or samples. Send your requirements for a quotation.Request a Quote
Jiangkai Casting logoJK CastingDrawing-based OEM metal parts

Material reference

ASTM A216 WCB Cast Steel: Equivalents, Composition and Properties

WCB is a cast carbon steel grade in ASTM A216/A216M, with up to 0.30% carbon and a tensile strength of 485–655 MPa. It is one of the most common cast steel callouts. This page gives its composition and tensile limits, the Chinese and Russian grades it is compared with, and what to put on an RFQ.

JK Casting · Buyer resource · Updated 16 November 2026

What WCB is

WCB is the middle grade of ASTM A216, the US specification for carbon steel castings. The standard has three grades: WCA, WCB and WCC. WCB allows up to 0.30% carbon and 1.00% manganese and requires a minimum yield strength of 250 MPa.

ASTM A216 is written for carbon steel castings for pressure-containing parts in high-temperature service, of a quality suitable for fusion welding to other castings or wrought steel. A grade callout names the material only: any certification or approval the part needs is a separate requirement and must be stated in the RFQ.

WCB equivalents: China and Russia

Scroll sideways to see the whole table

Approximate comparison. The standard on the drawing governs; substitution needs buyer approval.
GradeStandardMin. yield, MPaTensile, MPaMin. elongation, %How it compares
WCBASTM A216 (USA)250485–65522Reference grade
WCCASTM A216 (USA)275485–65522Higher minimum yield; lower carbon, more manganese allowed
ZG230-450GB/T 11352 (China)230450 min.22Lower minimum yield and tensile strength
ZG270-500GB/T 11352 (China)270500 min.18Higher minimum yield, lower minimum elongation
25ЛГОСТ 977 (Russia), normalised235441 min.19Lower minimum tensile strength (441 against 485 MPa)

These equivalents are approximate, not identical materials. Composition limits, test methods and heat treatment differ between standards. The standard named on the drawing governs, and any substitution needs the buyer’s written approval.

WCB chemical composition

Scroll sideways to see the whole table

ASTM A216/A216M-21, Table 1: maximum values.
ElementContent, % by mass
Carbon (C)≤0.30
Manganese (Mn)≤1.00
Phosphorus (P)≤0.035
Sulfur (S)≤0.035
Silicon (Si)≤0.60
Copper (Cu)≤0.30
Nickel (Ni)≤0.50
Chromium (Cr)≤0.50
Molybdenum (Mo)≤0.20
Vanadium (V)≤0.03

Values from ASTM A216/A216M-21, Table 1, all maximums. Copper, nickel, chromium, molybdenum and vanadium are specified residual elements; their total is 1.00% maximum unless Supplementary Requirement S50 is specified. For each 0.01% of carbon below the maximum, 0.04% more manganese is allowed, up to a limit set in the standard. Older editions allowed more phosphorus and sulfur, so check which edition the drawing cites.

WCB mechanical properties

Scroll sideways to see the whole table

ASTM A216/A216M-21, Table 2.
PropertyRequirement
Tensile strength, MPa485–655
Minimum yield strength, MPa250
Minimum elongation, %22
Minimum reduction of area, %35

Values from ASTM A216/A216M-21, Table 2. Elongation is measured over 50 mm (2 in). In ksi: tensile 70–95.

Heat treatment and welding

Heat treatment. ASTM A216 requires every casting to be heat treated and lists annealed, normalised, or normalised and tempered as the supply conditions. If the design needs one specific condition, state it on the drawing.

Welding. With carbon limited to 0.30%, WCB is a weldable carbon steel. Preheat and post-weld heat treatment depend on section thickness and the welding procedure; agree weld repair rules in the quality plan.

How JK Casting makes WCB castings

JK Casting makes carbon steel castings to customer drawings in Gaomi, Shandong, China. Parts are sand cast, including shell moulding in resin-coated sand, or made by lost-wax investment casting; investment castings made in-house weigh up to about 20 kg each. Castings are supplied raw or machined, and JK machines only the castings it makes. Each drawing is quoted separately, with tooling and unit price on separate lines.

For a quotation, send the drawing with the full grade designation and standard, the heat treatment condition and any tests the part needs. Material records such as EN 10204 3.1 certificates are provided when agreed for the order.

Related pages: Steel castings · Investment casting · Sand casting · What to put on a casting drawing · Send a drawing for quotation

Frequently asked questions

What is the Chinese equivalent of WCB?

No GB grade is identical. The nearest GB/T 11352 grades are ZG230-450 (230 MPa yield, 450 MPa tensile) and ZG270-500 (270 MPa yield, 500 MPa tensile, 18% elongation). WCB requires 250 MPa yield, 485–655 MPa tensile and 22% elongation, so a substitution needs approval.

What is the difference between WCB and WCC?

WCC allows less carbon (0.25% against 0.30%) and more manganese (1.20% against 1.00%) and requires a higher minimum yield strength (275 against 250 MPa). Both have a tensile range of 485–655 MPa and 22% minimum elongation.

What is the Russian equivalent of WCB?

ГОСТ 977 25Л is the usual approximate equivalent. Normalised, it requires 235 MPa yield, 441 MPa tensile and 19% elongation, which is below WCB’s 485 MPa minimum tensile strength.

Does a WCB callout include pressure-equipment certification?

No. WCB names the material grade and its properties. Any certification or approval the part needs is a separate requirement and must be stated in the RFQ.

Standards referenced: ASTM A216/A216M-21; GB/T 11352-2009; ГОСТ 977-88.