What WCC is
WCC is the strongest of the three ASTM A216 grades (WCA, WCB, WCC). It allows up to 0.25% carbon and 1.20% manganese and requires a minimum yield strength of 275 MPa, against 250 MPa for WCB. The tensile range and elongation are the same as WCB.
ASTM A216 is written for carbon steel castings for pressure-containing parts in high-temperature service, of a quality suitable for fusion welding to other castings or wrought steel. A grade callout names the material only: any certification or approval the part needs is a separate requirement and must be stated in the RFQ.
WCC equivalents and nearest grades
Scroll sideways to see the whole table
| Grade | Standard | Min. yield, MPa | Tensile, MPa | Min. elongation, % | How it compares |
|---|---|---|---|---|---|
| WCC | ASTM A216 (USA) | 275 | 485–655 | 22 | Reference grade |
| WCB | ASTM A216 (USA) | 250 | 485–655 | 22 | Lower minimum yield; more carbon, less manganese allowed |
| ZG270-500 | GB/T 11352 (China) | 270 | 500 min. | 18 | Similar minimum yield, lower minimum elongation |
| 25Л | ГОСТ 977 (Russia), normalised | 235 | 441 min. | 19 | Lower minimum yield and tensile strength |
These equivalents are approximate, not identical materials. Composition limits, test methods and heat treatment differ between standards. The standard named on the drawing governs, and any substitution needs the buyer’s written approval.
WCC chemical composition
Scroll sideways to see the whole table
| Element | Content, % by mass |
|---|---|
| Carbon (C) | ≤0.25 |
| Manganese (Mn) | ≤1.20 |
| Phosphorus (P) | ≤0.035 |
| Sulfur (S) | ≤0.035 |
| Silicon (Si) | ≤0.60 |
| Copper (Cu) | ≤0.30 |
| Nickel (Ni) | ≤0.50 |
| Chromium (Cr) | ≤0.50 |
| Molybdenum (Mo) | ≤0.20 |
| Vanadium (V) | ≤0.03 |
Values from ASTM A216/A216M-21, Table 1, all maximums. Copper, nickel, chromium, molybdenum and vanadium are specified residual elements; their total is 1.00% maximum unless Supplementary Requirement S50 is specified. For each 0.01% of carbon below the maximum, 0.04% more manganese is allowed, up to a limit set in the standard. Older editions allowed more phosphorus and sulfur, so check which edition the drawing cites.
WCC mechanical properties
Scroll sideways to see the whole table
| Property | Requirement |
|---|---|
| Tensile strength, MPa | 485–655 |
| Minimum yield strength, MPa | 275 |
| Minimum elongation, % | 22 |
| Minimum reduction of area, % | 35 |
Values from ASTM A216/A216M-21, Table 2. Elongation is measured over 50 mm (2 in). In ksi: tensile 70–95.
Heat treatment and welding
Heat treatment. ASTM A216 requires every casting to be heat treated and lists annealed, normalised, or normalised and tempered as the supply conditions. If the design needs one specific condition, state it on the drawing.
Welding. WCC has the lowest carbon limit of the A216 grades and is a weldable carbon steel. Preheat and post-weld heat treatment depend on section thickness and the welding procedure; agree weld repair rules in the quality plan.
How JK Casting makes WCC castings
JK Casting makes carbon steel castings to customer drawings in Gaomi, Shandong, China. Parts are sand cast, including shell moulding in resin-coated sand, or made by lost-wax investment casting; investment castings made in-house weigh up to about 20 kg each. Castings are supplied raw or machined, and JK machines only the castings it makes. Each drawing is quoted separately, with tooling and unit price on separate lines.
For a quotation, send the drawing with the full grade designation and standard, the heat treatment condition and any tests the part needs. Material records such as EN 10204 3.1 certificates are provided when agreed for the order.
Related pages: Steel castings · Investment casting · Sand casting · What to put on a casting drawing · Send a drawing for quotation
Frequently asked questions
What is the difference between WCB and WCC?
WCC allows less carbon (0.25% against 0.30%) and more manganese (1.20% against 1.00%) and requires a higher minimum yield strength (275 against 250 MPa). Both have a tensile range of 485–655 MPa and 22% minimum elongation.
Can WCB be supplied when the drawing calls for WCC?
Not without approval. WCB’s minimum yield strength (250 MPa) is below WCC’s 275 MPa, so the drawing’s grade governs and any substitution needs the buyer’s written approval.
What is the Chinese equivalent of WCC?
No GB grade is identical. ZG270-500 has a similar minimum yield (270 MPa) and a 500 MPa minimum tensile strength, but only 18% minimum elongation against WCC’s 22%.
Standards referenced: ASTM A216/A216M-21; GB/T 11352-2009; ГОСТ 977-88.