ZG270-500 Cast Steel (GB/T 11352): Equivalents, Composition and Properties

ZG270-500 is a cast carbon steel grade in China’s GB/T 11352: minimum yield strength 270 MPa, minimum tensile strength 500 MPa. Its former designation was ZG35. This page gives its composition and properties, how it compares with WCB and 35Л, and what to put on an RFQ.

JK Casting · Buyer resource · Updated 16 November 2026

What ZG270-500 is

In GB/T 11352 names, ZG stands for cast steel (铸钢); the first number is the minimum yield strength and the second the minimum tensile strength, both in MPa.

ZG270-500 is a higher-strength general engineering cast carbon steel with up to 0.40% carbon. It casts well and has good ductility, and is used for frames, bearing housings and other machine parts that carry higher loads. Its weldability is lower than that of ZG230-450 because of the higher carbon limit.

ZG270-500 equivalents: ASTM and ГОСТ

Scroll sideways to see the whole table

Approximate comparison. The standard on the drawing governs; substitution needs buyer approval.
GradeStandardMin. yield, MPaTensile, MPaMin. elongation, %How it compares
ZG270-500GB/T 11352 (China)270500 min.18Reference grade
WCBASTM A216 (USA)250485–65522Lower minimum yield, higher minimum elongation, tensile range 485–655
35ЛГОСТ 977 (Russia), normalised275491 min.15Similar minimum yield, lower minimum tensile strength and elongation
ZG230-450GB/T 11352 (China)230450 min.22The next GB grade down by strength

These equivalents are approximate, not identical materials. Composition limits, test methods and heat treatment differ between standards. The standard named on the drawing governs, and any substitution needs the buyer’s written approval.

ZG270-500 chemical composition

Scroll sideways to see the whole table

GB/T 11352-2009, Table 1: maximum values.
ElementContent, % by mass
Carbon (C)≤0.40
Silicon (Si)≤0.60
Manganese (Mn)≤0.90
Phosphorus (P)≤0.035
Sulfur (S)≤0.035
Nickel (Ni)≤0.40
Chromium (Cr)≤0.35
Copper (Cu)≤0.40
Molybdenum (Mo)≤0.20
Vanadium (V)≤0.05

Values from GB/T 11352-2009, Table 1, all maximums; nickel, chromium, copper, molybdenum and vanadium are residual elements. The 1989 edition set different silicon, phosphorus and sulfur limits, so check which edition the drawing cites.

ZG270-500 mechanical properties

Scroll sideways to see the whole table

GB/T 11352-2009: minimum values.
PropertyRequirement
Minimum tensile strength, MPa500
Minimum yield strength, MPa270
Minimum elongation, %18
Minimum reduction of area, %25

Values from GB/T 11352-2009. Impact values are agreed per contract and are left out here.

Heat treatment and welding

Heat treatment. GB/T 11352 carbon steel castings are normally supplied normalised, or normalised and tempered; annealing is also used. State the required condition on the drawing.

Welding. With up to 0.40% carbon, ZG270-500 needs more care in welding than ZG230-450; preheat and post-weld heat treatment depend on section thickness and the welding procedure.

How JK Casting makes ZG270-500 castings

JK Casting makes carbon steel castings to customer drawings in Gaomi, Shandong, China. Parts are sand cast, including shell moulding in resin-coated sand, or made by lost-wax investment casting; investment castings made in-house weigh up to about 20 kg each. Castings are supplied raw or machined, and JK machines only the castings it makes. Each drawing is quoted separately, with tooling and unit price on separate lines.

For a quotation, send the drawing with the full grade designation and standard, the heat treatment condition and any tests the part needs. Material records such as EN 10204 3.1 certificates are provided when agreed for the order.

Related pages: Steel castings · Investment casting · Sand casting · What to put on a casting drawing · Send a drawing for quotation

Frequently asked questions

Is WCB the same as ZG270-500?

Not exactly. WCB requires 250 MPa yield, 485–655 MPa tensile and 22% elongation; ZG270-500 requires 270 MPa yield, 500 MPa tensile and 18% elongation. They are approximate equivalents, so the drawing’s standard governs and a substitution needs approval.

What does ZG270-500 mean?

ZG stands for cast steel (铸钢). 270 is the minimum yield strength and 500 the minimum tensile strength, both in MPa, as set in GB/T 11352.

What is the Russian equivalent of ZG270-500?

ГОСТ 977 35Л is the nearest by strength: normalised, 275 MPa yield, 491 MPa tensile and 15% elongation, against 270 MPa, 500 MPa and 18% for ZG270-500. The equivalence is approximate.

Is ZG270-500 the same as ZG35?

ZG35 is the former designation of the grade. Current drawings name ZG270-500 together with its standard.

Standards referenced: GB/T 11352-2009; ASTM A216/A216M-21; ГОСТ 977-88.