35L (35Л) Cast Steel to ГОСТ 977: Equivalents, Composition and Properties

35Л (often written 35L) is a cast carbon steel grade in the Russian standard ГОСТ 977-88. 35 is the average carbon content in hundredths of a percent; Л marks a casting steel. This page gives its composition, properties and heat treatment and the grades it is compared with.

JK Casting · Buyer resource · Updated 16 November 2026

What 35Л is

35Л is an unalloyed structural casting steel in ГОСТ 977-88. 35 is the average carbon content in hundredths of a percent (carbon 0.32–0.40%); Л stands for литейная, casting steel. ГОСТ 977 sorts castings into groups 1–3 (general, responsible and especially responsible duty); the group sets the checks and the sulfur and phosphorus limits, so state it on the drawing.

35Л equivalents and nearest grades

Scroll sideways to see the whole table

Approximate comparison. The standard on the drawing governs; substitution needs buyer approval.
GradeStandardMin. yield, MPaTensile, MPaMin. elongation, %How it compares
35ЛГОСТ 977 (Russia), normalised275491 min.15Reference grade
ZG270-500GB/T 11352 (China)270500 min.18Similar minimum yield, higher minimum tensile strength and elongation
25ЛГОСТ 977 (Russia), normalised235441 min.19Lower carbon: lower strength, higher elongation

These equivalents are approximate, not identical materials. Composition limits, test methods and heat treatment differ between standards. The standard named on the drawing governs, and any substitution needs the buyer’s written approval.

35Л chemical composition

Scroll sideways to see the whole table

ГОСТ 977-88, Tables 1 and 4.
ElementContent, % by mass
Carbon (C)0.32–0.40
Manganese (Mn)0.45–0.90
Silicon (Si)0.20–0.52
Sulfur (S), groups 2 and 3≤0.045
Phosphorus (P), groups 2 and 3≤0.040
Sulfur (S), group 1≤0.050
Phosphorus (P), group 1≤0.050

Sulfur and phosphorus limits shown are for steel made by the basic process; ГОСТ 977 allows higher limits for acid and converter steel. Check the casting group and process stated for the order.

35Л mechanical properties

Scroll sideways to see the whole table

ГОСТ 977-88, Table 7: minimum values for castings with walls up to 100 mm.
ConditionMin. yield, MPaMin. tensile, MPaMin. elongation, %Min. reduction of area, %
Normalised, or normalised and tempered (К25)2754911525
Quenched and tempered (КТ35)3435401620

Impact values are left out of this table; if the part needs an impact test, state the test and temperature on the drawing.

Heat treatment and welding

Heat treatment. ГОСТ 977-88 gives these modes for 35Л: normalising at 860–880 °C and tempering at 600–630 °C, or quenching from 860–880 °C and tempering at 600–630 °C.

Welding. With up to 0.40% carbon, 35Л needs more care in welding than 25Л; preheat and post-weld heat treatment depend on section thickness and the welding procedure.

How JK Casting makes 35Л castings

JK Casting makes carbon steel castings to customer drawings in Gaomi, Shandong, China. Parts are sand cast, including shell moulding in resin-coated sand, or made by lost-wax investment casting; investment castings made in-house weigh up to about 20 kg each. Castings are supplied raw or machined, and JK machines only the castings it makes. Each drawing is quoted separately, with tooling and unit price on separate lines.

For a quotation, send the drawing with the full grade designation and standard, the heat treatment condition and any tests the part needs. Material records such as EN 10204 3.1 certificates are provided when agreed for the order.

Related pages: Steel castings · Investment casting · Sand casting · What to put on a casting drawing · Send a drawing for quotation

Frequently asked questions

What does 35Л mean?

35 is the average carbon content in hundredths of a percent (carbon 0.32–0.40%), and Л stands for литейная, a casting steel. The grade is defined in ГОСТ 977-88.

What are the equivalents of 35Л?

GB/T 11352 ZG270-500 is the grade usually compared with it: 270 MPa yield, 500 MPa tensile and 18% elongation, against 275 MPa, 491 MPa and 15% for normalised 35Л. The equivalence is approximate.

What is the chemical composition of 35Л?

Carbon 0.32–0.40%, manganese 0.45–0.90%, silicon 0.20–0.52%; sulfur and phosphorus limits depend on the casting group and steelmaking process, for example 0.045% sulfur and 0.040% phosphorus for basic-process steel in groups 2 and 3.

How is 35Л heat treated?

ГОСТ 977-88 gives normalising at 860–880 °C with tempering at 600–630 °C, or quenching from 860–880 °C with tempering at 600–630 °C. Normalised, the minimums are 275 MPa yield and 491 MPa tensile.