Custom castings from your drawings or samples. Send your requirements for a quotation.Request a Quote
Jiangkai Casting logoJK CastingDrawing-based OEM metal parts

Material reference

ASTM A352 LCB Cast Steel: Composition, Properties and Impact Test Temperature

LCB is a carbon steel grade in ASTM A352/A352M, the US specification for steel castings for pressure-containing parts in low-temperature service. Its usual minimum impact test temperature is −46 °C (−50 °F). This page gives its composition and tensile requirements and how it differs from WCB.

JK Casting · Buyer resource · Updated 16 November 2026

What LCB is

LCB is the carbon steel grade of ASTM A352, which covers ferritic and martensitic steel castings for pressure-containing parts intended primarily for low-temperature service. The standard lists −46 °C (−50 °F) as the usual minimum impact test temperature for LCB: the lowest temperature at which the material ordinarily must meet the impact requirements.

LCB compared with WCB

Scroll sideways to see the whole table

Approximate comparison. The standard on the drawing governs; substitution needs buyer approval.
GradeStandardMin. yield, MPaTensile, MPaMin. elongation, %How it compares
LCBASTM A352 (USA)240450–62024Reference grade
WCBASTM A216 (USA)250485–65522Same carbon and manganese limits, higher tensile range, no impact requirement in A216 Table 2
GP240GHEN 10213 (Europe)240420–60022Similar minimum yield, lower tensile range

These equivalents are approximate, not identical materials. Composition limits, test methods and heat treatment differ between standards. The standard named on the drawing governs, and any substitution needs the buyer’s written approval.

LCB chemical composition

Scroll sideways to see the whole table

ASTM A352/A352M-21, Table 1: maximum values.
ElementContent, % by mass
Carbon (C)≤0.30
Manganese (Mn)≤1.00
Phosphorus (P)≤0.04
Sulfur (S)≤0.045
Silicon (Si)≤0.60
Nickel (Ni)≤0.50
Chromium (Cr)≤0.50
Molybdenum (Mo)≤0.20
Copper (Cu)≤0.30
Vanadium (V)≤0.03

Nickel, chromium, molybdenum, copper and vanadium are residual elements with a total of 1.00% maximum. More manganese is allowed when carbon is below its maximum, up to a limit set in the standard.

LCB mechanical properties

Scroll sideways to see the whole table

ASTM A352/A352M-21, Table 2.
PropertyRequirement
Tensile strength, MPa450–620
Minimum yield strength, MPa240
Minimum elongation, %24
Minimum reduction of area, %35

In ksi: tensile 65–90, yield 35. Charpy impact energy values are set in Table 2 of ASTM A352; state the required test temperature and energy on the drawing or purchase order.

Heat treatment

Heat treatment. ASTM A352 requires ferritic castings such as LCB to be supplied normalised and tempered, or liquid quenched and tempered. Liquid quenching is normally needed to meet the properties in heavier sections.

How JK Casting makes LCB castings

JK Casting makes carbon steel castings to customer drawings in Gaomi, Shandong, China. Parts are sand cast, including shell moulding in resin-coated sand, or made by lost-wax investment casting; investment castings made in-house weigh up to about 20 kg each. Castings are supplied raw or machined, and JK machines only the castings it makes. Each drawing is quoted separately, with tooling and unit price on separate lines.

For a quotation, send the drawing with the full grade designation and standard, the heat treatment condition and any tests the part needs. Material records such as EN 10204 3.1 certificates are provided when agreed for the order.

Related pages: Steel castings · Investment casting · Sand casting · What to put on a casting drawing · Send a drawing for quotation

For LCB parts, state the impact test temperature and energy required; these are reviewed with the drawing before quoting.

Frequently asked questions

What is ASTM A352 LCB?

The carbon steel grade of ASTM A352, the specification for steel castings for pressure-containing parts in low-temperature service. Its usual minimum impact test temperature is −46 °C (−50 °F).

What is the difference between LCB and WCB?

Both allow up to 0.30% carbon and 1.00% manganese. LCB has a lower tensile range (450–620 MPa against 485–655 MPa) and higher minimum elongation (24% against 22%), and it is impact tested at a low temperature.

At what temperature is LCB impact tested?

ASTM A352 lists −46 °C (−50 °F) as the usual minimum test temperature for LCB. The energy values are set in Table 2 of the standard; state the required values on the order.

Standards referenced: ASTM A352/A352M-21; ASTM A216/A216M-21; EN 10213.